HOSTAFORM® S 9364 WS 10/1570 BLACK
 
HOSTAFORM S 9364 WS 10/1570 | POM | UV Resistant
 
Description
Preliminary Data Sheet
Hostaform® acetal copolymer grade S 9364 WS 10/1570 is a highly impact modified grade for demanding applications that also need improved resistance to UV exposure. Besides weatherability, Hostaform® S 9364 WS 10/1570 provides a significant improvement in impact strength and flexibility over standard impact modified grades such as Hostaform® S 9063 and S 9064. This grade is only available in black.
 
Chemical abbreviation according to ISO 1043-1: POM-HI
 
ISO Data Mechanical properties Value Unit Test Standard
Phys Density 1370 kg/m³ ISO 1183
Melt volume rate (MVR) 4.5 cm³/10min ISO 1133
MVR test temperature 190 ISO 1133
MVR test load 2.16 kg ISO 1133
Water absorption (23℃-sat) 0.8 % ISO 62
Mech Mechanical properties Value Unit Test Standard
Tensile modulus (1mm/min) 1500 MPa ISO 527-2/1A
Tensile stress at yield (50mm/min) 41 MPa ISO 527-2/1A
Tensile strain at yield (50mm/min) 20 % ISO 527-2/1A
Flexural modulus (23℃) 1400 MPa ISO 178
Charpy notched impact strength @ 23℃ 16 kJ/m² ISO 179/1eA
Charpy notched impact strength @ -30℃ 7 kJ/m² ISO 179/1eA
Therm Thermal properties Value Unit Test Standard
Melting temperature (10℃/min) 166 ISO 11357-1,-2,-3
DTUL @ 1.8 MPa 75 ISO 75-1/-2
Coeff.of linear therm. expansion (parallel) 1.2 E-4/℃ ISO 11359-2
Coeff.of linear therm. expansion (normal) 1.1 E-4/℃ ISO 11359-2
SpecProd Test specimen production Value Unit Test Standard
Processing conditions acc. ISO 9988-2 - Internal
 
Processing
Pre Drying
Drying is not normally required. If material has come in contact with moisture through improper storage or handling or through regrind use, drying to prevent splay and odor problems.
 
Drying time (h):3
Drying temperature (℃):80 - 100