进口塑胶料
注:请在右边的搜索栏查找产品

LNP STAT-KON PA66 RFD03

添加时间:2013-02-22  信息来源:http://www.simibc.com/  作者:苏州希普能塑料
LNP™ STAT-KON™ Compound PA66 RFD03
 
Also known as:LNP™ Stat-kon™ Compound RF-15 Product reorder name:RFD03
LNP* Stat-Kon* RFD03 is a Nylon 6/6 containing glass fiber.
 
Property
TYPICAL PROPERTIES(1)
MECHANICAL Value Unit Standard
Tensile Stress,yld,Type I,5mm/min 920 kgf/cm² ASTM D 638
Tensile Stress,brk,Type I,5mm/min 920 kgf/cm² ASTM D 638
Tensile Strain,yld,Type I,5mm/min 1.3 % ASTM D 638
Tensile Strain,brk,Type I,5mm/min 1.3 % ASTM D 638
Tensile Modulus,50mm/min 91000 kgf/cm² ASTM D 638
Flexural Stress,yld,1.3mm/min,50mm span 1800 kgf/cm² ASTM D 790
Flexural Stress,brk,1.3mm/min,50mm span 1820 kgf/cm² ASTM D 790
Flexural Modulus,1.3mm/min,50mm span 64600 kgf/cm² ASTM D 790
Tensile Stress,yield,5mm/min 92 MPa ISO 527
Tensile Stress,break,5mm/min 92 MPa ISO 527
Tensile Strain,yield,5mm/min 1.2 % ISO 527
Tensile Strain,break,5mm/min 1.2 % ISO 527
Tensile Modulus,1mm/min 8010 MPa ISO 527
Flexural Stress 134 MPa ISO 178
Flexural Modulus,2mm/min 6630 MPa ISO 178
IMPACT Value Unit Standard
Izod Impact,unnotched,23℃ 29 cm-kgf/cm ASTM D 4812
Izod Impact,notched,23℃ 5 cm-kgf/cm ASTM D 256
Multiaxial Impact 16 cm-kgf ISO 6603
Instrumented Impact Total Energy,23℃ 56 cm-kgf ASTM D 3763
Izod Impact,unnotched 80*10*4 +23℃ 18 kJ/m² ISO 180/1U
Izod Impact,notched 80*10*4 +23℃ 4 kJ/m² ISO 180/1A
THERMAL Value Unit Standard
HDT,0.45 MPa,3.2mm,unannealed 258 ASTM D 648
HDT,1.82 MPa,3.2mm,unannealed 247 ASTM D 648
CTE,-30℃ to 30℃,flow 3.00E-06 1/℃ ASTM D 696
CTE,-30℃ to 30℃,xflow 8.00E-06 1/℃ ASTM D 696
HDT/Bf,0.45 MPa Flatw 80*10*4 sp=64mm 258 ISO 75/Bf
HDT/Af,1.8 MPa Flatw 80*10*4 sp=64mm 245 ISO 75/Af
PHYSICAL Value Unit Standard
Specific Gravity 1.35 - ASTM D 792
Density 1.34 g/cm³ ASTM D 792
Moisture Absorption,50% RH,24 hrs 0.62 % ASTM D 570
Mold Shrinkage,flow,24 hrs(5) 0.5-0.8 % ASTM D 955
Mold Shrinkage,xflow,24 hrs(5) 1-3 % ASTM D 955
Moisture Absorption(23℃/50% RH) 0.99 % ISO 62
ELECTRICAL Value Unit Standard
Surface Resistivity 1.E+00-3.E+00 Ohm ASTM D 257
Source GMD,last updated:2012/05/02
Parameter Injection Molding Value Unit
Drying Temperature 80
Drying Time 4 hrs
Maximum Moisture Content 0.15-0.25 %
Melt Temperature 280-305
Front-Zone 3 Temperature 295-305
Middle-Zone 2 Temperature 280-295
Rear-Zone 1 Temperature 265-275
Mold Temperature 95-110
Back Pressure 0.2-0.3 MPa
Screw Speed 30-60 rpm
Source GMD,last updated:2012/05/02